Colibrium Additive Nickel 625 is the maker's Inconel 625 grade for laser powder bed fusion, here as-built, without post-print heat treatment. Rapid melt-pool solidification gives a fine cellular-dendritic structure, columnar grains along the build direction and niobium and molybdenum segregation at cell boundaries, making properties orientation-dependent. Parts carry high residual stress, are anchored to the plate by supports and have rough down-facing surfaces, so stress relief, plate removal and often hot isostatic pressing or solution annealing and machining follow. Printed parts serve as heat- and corrosion-resistant components with internal channels, such as heat exchangers and combustion hardware. Every value on this page is read from Colibrium Additive's own material data sheet — quoted, cited and dated — and is the maker's statement about printed material, not a measurement by MatWorld; none has yet been reviewed by a person.
Compliance & Regulations
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Elongation at Break(εf)4 entries | 40.00 | % | Balanced Parameter 140 – 400 W / 60 µm · as-built · ASTM E8 · XY | ||
| ↳ | 42.50 | % | Balanced Parameter 140 – 400 W / 60 µm · as-built · ASTM E8 · Z | ||
| ↳ | 37.00 | % | Surface Parameter 169 – 400 W / 30 µm · as-built · ASTM E8 · XY | ||
| ↳ | 42.50 | % | Surface Parameter 169 – 400 W / 30 µm · as-built · ASTM E8 · Z | ||
Hardness (Vickers)(HV)2 entries | 268 | HV | Balanced Parameter 140 – 400 W / 60 µm · as-built · XY | ||
| ↳ | 292 | HV | Surface Parameter 169 – 400 W / 30 µm · as-built · XY | ||
Ultimate Tensile Strength(σUTS)4 entries | 940.0 | MPa | Balanced Parameter 140 – 400 W / 60 µm · as-built · ASTM E8 · XY | ||
| ↳ | 880.0 | MPa | Balanced Parameter 140 – 400 W / 60 µm · as-built · ASTM E8 · Z | ||
| ↳ | 980.0 | MPa | Surface Parameter 169 – 400 W / 30 µm · as-built · ASTM E8 · XY | ||
| ↳ | 890.0 | MPa | Surface Parameter 169 – 400 W / 30 µm · as-built · ASTM E8 · Z | ||
Yield Strength (0.2% offset)(σy)4 entries | 640.0 | MPa | Balanced Parameter 140 – 400 W / 60 µm · as-built · ASTM E8 · XY | ||
| ↳ | 575.0 | MPa | Balanced Parameter 140 – 400 W / 60 µm · as-built · ASTM E8 · Z | ||
| ↳ | 710.0 | MPa | Surface Parameter 169 – 400 W / 30 µm · as-built · ASTM E8 · XY | ||
| ↳ | 625.0 | MPa | Surface Parameter 169 – 400 W / 30 µm · as-built · ASTM E8 · Z | ||
Young's Modulus(E)4 entries | 178.0 | GPa | Balanced Parameter 140 – 400 W / 60 µm · as-built · ASTM E8 · XY | ||
| ↳ | 133.0 | GPa | Balanced Parameter 140 – 400 W / 60 µm · as-built · ASTM E8 · Z | ||
| ↳ | 168.0 | GPa | Surface Parameter 169 – 400 W / 30 µm · as-built · ASTM E8 · XY | ||
| ↳ | 138.0 | GPa | Surface Parameter 169 – 400 W / 30 µm · as-built · ASTM E8 · Z |
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Density(ρ) | 8.442 | kg/m³ | 22°C |
Reference data from cited sources. Not verified or certified by MatWorld Inc. Verify against the source before use in design. Terms: engineering data