5083 Aluminum is a non-heat-treatable Al-Mg alloy (approximately 4.4% Mg) with excellent seawater corrosion resistance, used primarily in marine structures, shipbuilding, and chemical storage applications. The O temper is fully annealed, providing maximum ductility and formability with minimum strength, making it suitable for applications requiring extensive cold-working or complex forming operations.
Compliance & Regulations
13 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Ultimate Bearing Strength(Fbru)4 entries | 60.00 | ksi | 22°C · Sheet/Plate · O · AMS 4056 OR AMS-QQ-A-250/6 · t=0.051-1.500 in · e/D=1.5 | ||
| ↳ | 62.00 | ksi | 22°C · Sheet/Plate · O · AMS 4056 OR AMS-QQ-A-250/6 · t=0.051-1.500 in · e/D=1.5 | ||
| ↳ | 76.00 | ksi | 22°C · Sheet/Plate · O · AMS 4056 OR AMS-QQ-A-250/6 · t=0.051-1.500 in · e/D=2 | ||
| ↳ | 78.00 | ksi | 22°C · Sheet/Plate · O · AMS 4056 OR AMS-QQ-A-250/6 · t=0.051-1.500 in · e/D=2 | ||
Bearing Yield Strength(Fbry)4 entries | 32.00 | ksi | 22°C · Sheet/Plate · O · AMS 4056 OR AMS-QQ-A-250/6 · t=0.051-1.500 in · e/D=1.5 | ||
| ↳ | 34.00 | ksi | 22°C · Sheet/Plate · O · AMS 4056 OR AMS-QQ-A-250/6 · t=0.051-1.500 in · e/D=1.5 | ||
| ↳ | 38.00 | ksi | 22°C · Sheet/Plate · O · AMS 4056 OR AMS-QQ-A-250/6 · t=0.051-1.500 in · e/D=2 | ||
| ↳ | 40.00 | ksi | 22°C · Sheet/Plate · O · AMS 4056 OR AMS-QQ-A-250/6 · t=0.051-1.500 in · e/D=2 | ||
Compressive Modulus(Ec) | 10,400 | ksi | 22°C · Sheet/Plate | ||
Compressive Tangent Modulus vs Stress(Etn(σ))4 entries | Curve (11 pts) | ksi | 21°C · L | ||
| ↳ | Curve (11 pts) | ksi | 21°C · LT | ||
| ↳ | Curve (14 pts) | ksi | 21°C · L | ||
| ↳ | Curve (14 pts) | ksi | 21°C · LT | ||
Compressive Yield Strength(Fcy)4 entries | 18.00 | ksi | 22°C · Sheet/Plate · O · AMS 4056 OR AMS-QQ-A-250/6 · L · t=0.051-1.500 in | ||
| ↳ | 19.00 | ksi | 22°C · Sheet/Plate · O · AMS 4056 OR AMS-QQ-A-250/6 · L · t=0.051-1.500 in | ||
| ↳ | 18.00 | ksi | 22°C · Sheet/Plate · O · AMS 4056 OR AMS-QQ-A-250/6 · LT · t=0.051-1.500 in | ||
| ↳ | 19.00 | ksi | 22°C · Sheet/Plate · O · AMS 4056 OR AMS-QQ-A-250/6 · LT · t=0.051-1.500 in | ||
Elongation at Break(εf) | 12.00 – 16.00 | - | 8 entriesClick to expand | ||
Poisson's Ratio(ν) | 0.3300 | - | 22°C | ||
Shear Modulus(G) | 3,350 | ksi | 22°C · Extrusion | ||
Ultimate Shear Strength(Fsu)2 entries | 25.00 | ksi | 22°C · Sheet/Plate · O · AMS 4056 OR AMS-QQ-A-250/6 · t=0.051-1.500 in | ||
| ↳ | 26.00 | ksi | 22°C · Sheet/Plate · O · AMS 4056 OR AMS-QQ-A-250/6 · t=0.051-1.500 in | ||
Stress–Strain Curve(σ–ε) | Curve (16 pts) | ksi | 21°C · L | ||
Stress–Strain Curve (buckling region, ≤ 2% strain)(σ–ε (low-strain)) | — | ksi | 8 entriesClick to expand | ||
Ultimate Tensile Strength(σUTS) | 36.00 – 41.00 | ksi | 10 entriesClick to expand | ||
Yield Strength (0.2% offset)(σy) | 14.00 – 19.00 | ksi | 10 entriesClick to expand | ||
Young's Modulus(E) | 10,200 | ksi | 22°C · Sheet/Plate | ||
2 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
CTE vs Temperature(α(T)) | Curve (9 pts) | µin/in·°F | — | ||
Thermal Conductivity vs Temperature(k(T)) | Curve (20 pts) | BTU/(hr·ft·°F) | — |
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Density(ρ) | 0.09600 | lb/in³ | 22°C |