316L stainless steel is a low-carbon austenitic stainless steel alloyed with molybdenum, designed to resist corrosion in severely aggressive environments—particularly chloride-bearing and acidic media. It is widely used in chemical processing, offshore oil and gas, pharmaceutical manufacturing, and food processing where both corrosion resistance and ease of welding are critical; the low carbon content minimizes carbide precipitation during welding, making it superior to standard 316 for applications involving repeated thermal cycling or extended service in corrosive solutions.
Compliance & Regulations
10 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Elongation at Break(εf) | 40.00 – 45.00 | % | 10 entriesClick to expand | ||
Stress–Strain Curve(σ–ε) | — | ksi | 8 entriesClick to expand | ||
Ultimate Tensile Strength(σUTS) | 70.34 | ksi | values according to ASTM A240 · minimum · Sheet/Plate · ASTM A240 | ||
Yield Strength (0.2% offset)(σy)4 entries | 24.66 | ksi | values according to ASTM A240 · minimum · Sheet/Plate · ASTM A240 | ||
| ↳ | 34.81 | ksi | 20°C · values according to EN 10088-2 · minimum · cold rolled coil and sheet (C) · EN 10088-2 | ||
| ↳ | 31.91 | ksi | 20°C · values according to EN 10088-2 · minimum · quarto plate (P) · EN 10088-2 | ||
| ↳ | 31.91 | ksi | 20°C · values according to EN 10088-2 · minimum · hot rolled coil and sheet (H) · EN 10088-2 | ||
Yield Strength vs Temperature(σy(T)) | Curve (4 pts) | ksi | specimen ASTM A370 round, 0.350 in. diameter, longitudinal | ||
Young's Modulus(E) | 29,007.5 | ksi | 20°C · EN 10088-1 | ||
Young's Modulus vs Temperature(E(T)) | Curve (29 pts) | ksi | notes | ||
7 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
CTE vs Temperature(α(T)) | Curve (15 pts) | µin/in·°F | notes | ||
Maximum Service Temperature(Tmax) | 849.9 | °F | Section VIII, Division 1 applications · ASME Boiler and Pressure Vessel Code | ||
Specific Heat vs Temperature(Cp(T))3 entries | Curve (15 pts) | BTU/(lb·°F) | notes | ||
| ↳ | Curve (40 pts) | BTU/(lb·°F) | notes | ||
| ↳ | Curve (39 pts) | BTU/(lb·°F) | notes | ||
Thermal Conductivity(k) | 8.667 | BTU/(hr·ft·°F) | 20°C · EN 10088-1 | ||
Thermal Conductivity vs Temperature(k(T))2 entries | Curve (15 pts) | BTU/(hr·ft·°F) | notes | ||
| ↳ | Curve (30 pts) | BTU/(hr·ft·°F) | notes | ||
Thermal Diffusivity(α) | Curve (15 pts) | BTU/(hr·ft·°F) | notes | ||
Coefficient of Thermal Expansion(α (CTE)) | 8.889 | µin/in·°F | 20–100 °C · EN 10088-1 |
2 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Density(ρ) | 0.2890 | lb/in³ | EN 10088-1 | ||
Density vs Temperature(ρ(T))2 entries | Curve (15 pts) | lb/in³ | notes | ||
| ↳ | Curve (15 pts) | lb/in³ | notes |
1 interactive curve for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Electrical Resistivity(ρe)2 entries | 7.500e-7 | Ω·m | 20°C · EN 10088-1 | ||
| ↳ | Curve (15 pts) | Ω·m | notes |
Reference data from cited sources. Not verified or certified by MatWorld Inc. Verify against the source before use in design. Terms: engineering data