316L stainless steel made by bound metal deposition is the low-carbon, molybdenum-alloyed austenitic grade, printed from metal-filled polymer filament and then debound and sintered into metal. The green part is printed oversize to allow for sintering shrinkage, and supports or a ceramic interface layer are often needed to limit distortion in the furnace. Sintered parts are largely dense but can keep fine residual porosity, with layer lines and some anisotropy between build directions. Critical surfaces are usually machined or polished. Typical uses are corrosion-resistant fixtures, tooling, housings and low-volume fluid-handling parts.
Compliance & Regulations
Each row is one condition this material was measured in. Its values and curves are in the tables and charts below, labelled with the condition; the ranges here span that row's own cited values and are never averaged across rows.
| Condition | Yield (MPa) | UTS (MPa) | Elongation (%) | Density (kg/m³) | Values | Curves |
|---|---|---|---|---|---|---|
| Desktop Metal 316L Stainless Steel (Studio System 2), sintered | 169–222 | 533–585 | 65.0–79.0 | 7740–7820 | 8 | 0 |
| Markforged 316L Stainless Steel, sintered | 170 | 465 | 44.0 | — | 3 | 0 |
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Charpy Impact Energy(KV) | 219 range 209–229 | J | Desktop Metal 316L Stainless Steel (Studio System 2), sintered · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · sintered · MPIF 59 | ||
Elongation at Break(εf)3 entries | 72.00 range 65.00–79.00 | % | Desktop Metal 316L Stainless Steel (Studio System 2), sintered · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · sintered · ASTM E8M | ||
| ↳ | 66.00 | % | Desktop Metal 316L Stainless Steel (Studio System 2), sintered · MECHANICAL PROPERTIES SINTERED IN DESKTOP METAL FURNACE · sintered · ASTM E8M | ||
| ↳ | 44.00 | % | Markforged 316L Stainless Steel, sintered · sintered · ASTM E8 | ||
Ultimate Tensile Strength(σUTS)3 entries | 580.0 range 575.0–585.0 | MPa | Desktop Metal 316L Stainless Steel (Studio System 2), sintered · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · sintered · ASTM E8M | ||
| ↳ | 533.0 | MPa | Desktop Metal 316L Stainless Steel (Studio System 2), sintered · MECHANICAL PROPERTIES SINTERED IN DESKTOP METAL FURNACE · sintered · ASTM E8M | ||
| ↳ | 465.0 | MPa | Markforged 316L Stainless Steel, sintered · sintered · ASTM E8 | ||
Yield Strength (0.2% offset)(σy)3 entries | 210.0 range 198.0–222.0 | MPa | Desktop Metal 316L Stainless Steel (Studio System 2), sintered · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · sintered · ASTM E8M | ||
| ↳ | 169.0 | MPa | Desktop Metal 316L Stainless Steel (Studio System 2), sintered · MECHANICAL PROPERTIES SINTERED IN DESKTOP METAL FURNACE · sintered · ASTM E8M | ||
| ↳ | 170.0 | MPa | Markforged 316L Stainless Steel, sintered · sintered · ASTM E8 |
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Density(ρ)2 entries | 7.780 range 7.740–7.820 | kg/m³ | Desktop Metal 316L Stainless Steel (Studio System 2), sintered · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · sintered | ||
| ↳ | 8.000 | kg/m³ | — | — |
Reference data from cited sources. Not verified or certified by MatWorld Inc. Verify against the source before use in design. Terms: engineering data
Machines the manufacturer states for this material.