Ti-6Al-2Sn-4Zr-2Mo is a near-alpha titanium alloy with aluminum, tin, zirconium, and molybdenum additions designed for elevated temperature applications requiring creep resistance and thermal stability. The annealed condition provides optimal combination of strength retention at intermediate temperatures (up to ~300°C), good fracture toughness, and formability in sheet form for aerospace engines, compressor blades, and casings.
Compliance & Regulations
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Compressive Modulus(Ec) | 124.1 | GPa | 22°C · Sheet | ||
Elongation at Break(εf) | 15.00 | % | — | ||
Poisson's Ratio(ν) | 0.3200 | - | 22°C | ||
Shear Modulus(G) | 42.75 | GPa | 22°C · Sheet | ||
Ultimate Tensile Strength(σUTS)2 entries | 999.7 | MPa | 22°C · Sheet · Triplex annealed · AMS-T-9046, Comp. AB-4 · L · t=≤0.187 in | ||
| ↳ | 999.7 | MPa | 22°C · Sheet · Triplex annealed · AMS-T-9046, Comp. AB-4 · LT · t=≤0.187 in | ||
Yield Strength (0.2% offset)(σy)2 entries | 930.8 | MPa | 22°C · Sheet · Triplex annealed · AMS-T-9046, Comp. AB-4 · L · t=≤0.187 in | ||
| ↳ | 930.8 | MPa | 22°C · Sheet · Triplex annealed · AMS-T-9046, Comp. AB-4 · LT · t=≤0.187 in | ||
Young's Modulus(E) | 114.0 | GPa | — |
3 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
CTE vs Temperature(α(T)) | Curve (6 pts) | 1/K | Duplex annealed | ||
Maximum Service Temperature(Tmax) | 811 | K | — | ||
Specific Heat vs Temperature(Cp(T)) | Curve (5 pts) | J/(kg·K) | Duplex annealed | ||
Thermal Conductivity vs Temperature(k(T)) | Curve (5 pts) | W/(m·K) | Duplex annealed |
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Density(ρ) | 4.540 | g/cm³ | — |