UltiMaker PC is a polycarbonate filament grade printed by fused deposition modeling, here in the conditioned state, equilibrated with ambient humidity rather than tested dry off the printer. Polycarbonate needs high nozzle and bed temperatures and an enclosed build space, because its shrinkage on cooling causes warping and residual stress, and the filament must be dried before printing. Printed parts are anisotropic and weakest across the layer interfaces, with visible layer lines and none of the optical clarity of molded PC. They are used as tough functional prototypes, jigs, fixtures, housings and parts exposed to moderate heat. Every value on this page is read from UltiMaker's own material data sheet — quoted, cited and dated — and is the maker's statement about printed material, not a measurement by MatWorld; none has yet been reviewed by a person.
Compliance & Regulations
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Notched Charpy Impact Strength(acN) | 11.60 range 10.20–13.00 | kJ/m² | 23°C · conditioned · ISO 179-1 / 1eB · XY | ||
Elongation at Break(εf)3 entries | 9.200 range 8.300–10.10 | % | conditioned · ASTM D3039 · XY | ||
| ↳ | 6.700 range 6.400–7.000 | % | YZ (Side) · conditioned · ASTM D3039 | ||
| ↳ | 2.000 range 1.900–2.100 | % | conditioned · ASTM D3039 · Z | ||
Flexural Modulus(Ef)3 entries | 234.8 range 223.1–246.6 | ksi | conditioned · ISO 178 · XY | ||
| ↳ | 297.6 range 283.8–311.4 | ksi | YZ (Side) · conditioned · ISO 178 | ||
| ↳ | 294.7 range 288.5–301 | ksi | conditioned · ISO 178 · Z | ||
Flexural Strength (MOR)(σf)3 entries | 12.97 range 12.63–13.30 | ksi | conditioned · ISO 178 · XY | ||
| ↳ | 14.27 range 13.76–14.78 | ksi | YZ (Side) · conditioned · ISO 178 | ||
| ↳ | 4.685 range 4.148–5.221 | ksi | conditioned · ISO 178 · Z | ||
Hardness (Shore D)(Shore D) | 81.00 | Shore D | conditioned · ISO 7619-1 · XY | ||
Ultimate Tensile Strength(σUTS)3 entries | 6.266 range 6.048–6.483 | ksi | conditioned · ASTM D3039 · XY | ||
| ↳ | 7.948 range 7.803–8.093 | ksi | YZ (Side) · conditioned · ASTM D3039 | ||
| ↳ | 3.655 range 3.350–3.960 | ksi | conditioned · ASTM D3039 · Z | ||
Yield Strength (0.2% offset)(σy)2 entries | 7.731 range 7.556–7.905 | ksi | conditioned · ASTM D3039 · XY | ||
| ↳ | 8.485 range 8.354–8.615 | ksi | YZ (Side) · conditioned · ASTM D3039 | ||
Young's Modulus(E)3 entries | 347.2 range 333–361.4 | ksi | conditioned · ASTM D3039 · XY | ||
| ↳ | 341.1 range 330–352.3 | ksi | YZ (Side) · conditioned · ASTM D3039 | ||
| ↳ | 327.1 range 315.9–338.2 | ksi | conditioned · ASTM D3039 · Z |
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Glass Transition Temperature(Tg) | 278.1 | °F | — | ||
Heat Deflection Temperature(HDT) | 220.1 range 218.8–221.3 | °F | 0.45 MPa load · conditioned · ISO 75-2 / B | ||
Melting Point / Solidus(Tm) | 433.5 | °F | — | ||
Vicat Softening Temperature(VST) | 238.4 range 237.7–239.2 | °F | conditioned · ISO 306 / A120 |
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Density(ρ) | 0.04335 | lb/in³ | — | — |
Reference data from cited sources. Not verified or certified by MatWorld Inc. Verify against the source before use in design. Terms: engineering data