Inconel 600 is a nickel-chromium superalloy with excellent oxidation and corrosion resistance up to 1100°C, used in high-temperature applications including aerospace engines, chemical processing, and nuclear reactors. The hot-worked condition provides good strength and ductility with moderate work hardening, suitable for applications requiring both elevated-temperature capability and fabricability in round, square, hexagonal, and rectangular forms per ASTM B166.
Compliance & Regulations
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Compressive Modulus(Ec) | 3,000 | ksi | 22°C · Sheet/Strip/Plate | ||
Elongation at Break(εf)3 entries | 20.00 | - | 22°C · Round · Hot-worked · ASTM B166 · L · t=0.250-0.500 in | ||
| ↳ | 25.00 | - | 22°C · Round · Hot-worked · ASTM B166 · L · t=0.501-3.000 in | ||
| ↳ | 30.00 | - | 22°C · Round · Hot-worked · ASTM B166 · L · t=>3.000 in | ||
Poisson's Ratio(ν) | 0.2900 | - | 22°C | ||
Shear Modulus(G) | 11,000 | ksi | 22°C · Round | ||
Ultimate Tensile Strength(σUTS)4 entries | 85.00 | ksi | 22°C · Round · Hot-worked · ASTM B166 · L · t=>3.000 in | ||
| ↳ | 85.00 | ksi | 22°C · Square, hexagon, and rectangle · Hot-worked · ASTM B166 · L · t=All in | ||
| ↳ | 95.00 | ksi | 22°C · Round · Hot-worked · ASTM B166 · L · t=0.250-0.500 in | ||
| ↳ | 90.00 | ksi | 22°C · Round · Hot-worked · ASTM B166 · L · t=0.501-3.000 in | ||
Yield Strength (0.2% offset)(σy)4 entries | 45.00 | ksi | 22°C · Round · Hot-worked · ASTM B166 · L · t=0.250-0.500 in | ||
| ↳ | 40.00 | ksi | 22°C · Round · Hot-worked · ASTM B166 · L · t=0.501-3.000 in | ||
| ↳ | 35.00 | ksi | 22°C · Round · Hot-worked · ASTM B166 · L · t=>3.000 in | ||
| ↳ | 35.00 | ksi | 22°C · Square, hexagon, and rectangle · Hot-worked · ASTM B166 · L · t=All in | ||
Young's Modulus(E) | 3,000 | ksi | 22°C · Sheet/Strip/Plate |
3 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
CTE vs Temperature(α(T)) | Curve (17 pts) | µin/in·°F | — | ||
Specific Heat vs Temperature(Cp(T)) | Curve (17 pts) | BTU/(lb·°F) | — | ||
Thermal Conductivity vs Temperature(k(T)) | Curve (17 pts) | BTU/(hr·ft·°F) | — |
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Density(ρ) | 0.3040 | lb/in³ | 22°C |