Commercially pure titanium (CP-Ti) in annealed condition is an unalloyed titanium grade offering excellent corrosion resistance and biocompatibility with moderate strength suitable for applications requiring ductility and formability. Primary uses include aerospace components, chemical processing equipment, and medical implants; the annealed condition provides optimal ductility and fracture toughness with yield strengths typically 25–50 ksi and elongation exceeding 20% across available forms (bar, sheet, plate, and extruded shapes).
Compliance & Regulations
16 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Ultimate Bearing Strength(Fbru)3 entries | 120 | ksi | 22°C · Sheet/Strip/Plate · Annealed · AMS 4901 OR AMS-T-9046 · t=≤1.000 in · e/D=1.5 | ||
| ↳ | Curve (13 pts) | ksi | — | ||
| ↳ | Curve (11 pts) | ksi | — | ||
Bearing Yield Strength(Fbry)3 entries | 101 | ksi | 22°C · Sheet/Strip/Plate · Annealed · AMS 4901 OR AMS-T-9046 · t=≤1.000 in · e/D=1.5 | ||
| ↳ | Curve (12 pts) | ksi | — | ||
| ↳ | Curve (13 pts) | ksi | — | ||
Compressive Modulus(Ec) | 16,000 | ksi | 22°C · Sheet/Strip/Plate | ||
Compressive Yield Strength(Fcy)4 entries | 70.00 | ksi | 22°C · Sheet/Strip/Plate · Annealed · AMS 4901 OR AMS-T-9046 · L · t=≤1.000 in | ||
| ↳ | 70.00 | ksi | 22°C · Sheet/Strip/Plate · Annealed · AMS 4901 OR AMS-T-9046 · LT · t=≤1.000 in | ||
| ↳ | Curve (14 pts) | ksi | L | ||
| ↳ | Curve (17 pts) | ksi | L | ||
Elongation at Break(εf) | 15.00 – 24.00 | - | 13 entriesClick to expand | ||
Reduction of Area(RA) | 30.00 | - | 5 entriesClick to expand | ||
Shear Modulus(G) | 6,500 | ksi | 22°C · Sheet/Strip/Plate | ||
Ultimate Shear Strength(Fsu)3 entries | 42.00 | ksi | 22°C · Sheet/Strip/Plate · Annealed · AMS 4901 OR AMS-T-9046 · t=≤1.000 in | ||
| ↳ | Curve (11 pts) | ksi | — | ||
| ↳ | Curve (11 pts) | ksi | — | ||
Stress–Strain Curve(σ–ε)4 entries | Curve (22 pts) | ksi | 21°C · L | ||
| ↳ | Curve (22 pts) | ksi | 21°C · LT | ||
| ↳ | Curve (20 pts) | ksi | 21°C · L | ||
| ↳ | Curve (20 pts) | ksi | 21°C · LT | ||
Ultimate Tensile Strength(σUTS) | 35.00 – 80.00 | ksi | 16 entriesClick to expand | ||
Yield Strength (0.2% offset)(σy) | 25.00 – 70.00 | ksi | 16 entriesClick to expand | ||
Young's Modulus(E) | 15,500 | ksi | 22°C · Sheet/Strip/Plate | ||
3 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
CTE vs Temperature(α(T)) | Curve (4 pts) | µin/in·°F | — | ||
Specific Heat vs Temperature(Cp(T)) | Curve (7 pts) | BTU/(lb·°F) | — | ||
Thermal Conductivity vs Temperature(k(T)) | Curve (13 pts) | BTU/(hr·ft·°F) | — |
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Density(ρ) | 0.1630 | lb/in³ | 22°C |