7475-T761 is a high-strength aluminum-zinc-magnesium-copper alloy reinforced with aramid fibers in sheet laminate form, delivering enhanced damage tolerance and fatigue resistance for aerospace structural applications. The T761 temper (overaged condition) provides controlled strength levels with improved fracture toughness relative to peak-hardness tempers, making it suitable for damage-critical aircraft components operating at intermediate temperatures.
Compliance & Regulations
32 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Ultimate Bearing Strength(Fbru)2 entries | 91.00 | ksi | 22°C · Aramid fiber reinforced sheet laminate · AMS 4302 · L | ||
| ↳ | 96.00 | ksi | 22°C · Aramid fiber reinforced sheet laminate · AMS 4302 · LT | ||
Bearing Yield Strength(Fbry)2 entries | 73.00 | ksi | 22°C · Aramid fiber reinforced sheet laminate · AMS 4302 · L | ||
| ↳ | 76.00 | ksi | 22°C · Aramid fiber reinforced sheet laminate · AMS 4302 · LT | ||
Compressive Modulus(Ec) | 9,600 | ksi | 22°C · Aramid fiber reinforced sheet laminate | ||
Compressive Tangent Modulus vs Stress(Etn(σ)) | — | ksi | 8 entriesClick to expand | ||
Compressive Yield Strength(Fcy)2 entries | 46.00 | ksi | 22°C · Aramid fiber reinforced sheet laminate · AMS 4302 · L | ||
| ↳ | 51.00 | ksi | 22°C · Aramid fiber reinforced sheet laminate · AMS 4302 · LT | ||
Elongation at Break(εf)2 entries | 1.500 | % | 22°C · Aramid fiber reinforced sheet laminate · AMS 4302 · L | ||
| ↳ | 6.100 | % | 22°C · Aramid fiber reinforced sheet laminate · AMS 4302 · LT | ||
Poisson's Ratio(ν) | 0.3500 | - | 22°C | ||
Shear Modulus(G) | 2,800 | ksi | 22°C · Aramid fiber reinforced sheet laminate | ||
Ultimate Shear Strength(Fsu) | 35.00 | ksi | 22°C · Aramid fiber reinforced sheet laminate · AMS 4302 | ||
Stress–Strain Curve(σ–ε) | — | ksi | 7 entriesClick to expand | ||
Stress–Strain Curve (buckling region, ≤ 2% strain)(σ–ε (low-strain)) | — | ksi | 17 entriesClick to expand | ||
Ultimate Tensile Strength(σUTS)2 entries | 103 | ksi | 22°C · Aramid fiber reinforced sheet laminate · AMS 4302 · L | ||
| ↳ | 56.00 | ksi | 22°C · Aramid fiber reinforced sheet laminate · AMS 4302 · LT | ||
Yield Strength (0.2% offset)(σy)2 entries | 76.00 | ksi | 22°C · Aramid fiber reinforced sheet laminate · AMS 4302 · L | ||
| ↳ | 48.00 | ksi | 22°C · Aramid fiber reinforced sheet laminate · AMS 4302 · LT | ||
Young's Modulus(E) | 9,800 | ksi | 22°C · Aramid fiber reinforced sheet laminate | ||
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Density(ρ) | 0.08500 | lb/in³ | 22°C |
Reference data from cited sources. Not verified or certified by MatWorld Inc. Verify against the source before use in design. Terms: engineering data