5454 Aluminum H34

Verifiedmetal
UNS A95454

5454 aluminum alloy is a non-heat-treatable Al-Mg system (3–5% Mg) offering excellent seawater corrosion resistance and weldability, commonly used in marine and chemical handling applications. The H34 temper (strain-hardened and partially annealed) provides moderate strength with maintained ductility, suitable for sheet and plate fabrication where corrosion resistance and formability are prioritized over maximum strength.

aerospacestructural

Compliance & Regulations

?Conflict Free?FDA?RoHS?REACH?TSCA?Prop 65
5454 Aluminum/5454 Aluminum H34
Property OverviewNormalized to typical max values
Filter by
Form
e/D Ratio
Orientation
PropertyValueUnitConditionsSource
Ultimate Bearing Strength(Fbru)2 entries
57.00
ksi22°C · Sheet/Plate · H34 · AMS-QQ-A-250/10 · t=0.020-1.000 in · e/D=1.5
78.00
ksi22°C · Sheet/Plate · H34 · AMS-QQ-A-250/10 · t=0.020-1.000 in · e/D=2
Bearing Yield Strength(Fbry)2 entries
41.00
ksi22°C · Sheet/Plate · H34 · AMS-QQ-A-250/10 · t=0.020-1.000 in · e/D=1.5
49.00
ksi22°C · Sheet/Plate · H34 · AMS-QQ-A-250/10 · t=0.020-1.000 in · e/D=2
Compressive Modulus(Ec)
Curve (19 pts)
ksi
Compressive Tangent Modulus vs Stress(Etn(σ))2 entries
Curve (12 pts)
ksi21°C · L
Curve (11 pts)
ksi21°C · LT
Compressive Yield Strength(Fcy)2 entries
27.00
ksi22°C · Sheet/Plate · H34 · AMS-QQ-A-250/10 · L · t=0.020-1.000 in
29.00
ksi22°C · Sheet/Plate · H34 · AMS-QQ-A-250/10 · LT · t=0.020-1.000 in
Poisson's Ratio(ν)
0.3300
-22°C
Shear Modulus(G)
3,850
ksi22°C · Sheet/Plate
Ultimate Shear Strength(Fsu)
23.00
ksi22°C · Sheet/Plate · H34 · AMS-QQ-A-250/10 · t=0.020-1.000 in
Stress–Strain Curve (buckling region, ≤ 2% strain)(σ–ε (low-strain))
ksi5 entriesClick to expand
Ultimate Tensile Strength(σUTS)
39.00 ksi11 entriesClick to expand
Yield Strength (0.2% offset)(σy)2 entries
29.00
ksi22°C · Sheet/Plate · H34 · AMS-QQ-A-250/10 · L · t=0.020-1.000 in
28.00
ksi22°C · Sheet/Plate · H34 · AMS-QQ-A-250/10 · LT · t=0.020-1.000 in
Young's Modulus(E)
10,200
ksi22°C · Sheet/Plate
N entriesMultiple entries per property — large groups are collapsed; click a summary row to expand. Use filters above to narrow by form / heat treatment / basis.
Rows with are inherited from the base material
Verified Unverified Low confidence (<80%) Link to source
PropertyValueUnitConditionsSource
CTE vs Temperature(α(T))
Curve (17 pts)
µin/in·°F
Thermal Conductivity vs Temperature(k(T))
Curve (20 pts)
BTU/(hr·ft·°F)
Rows with are inherited from the base material
Verified Unverified Low confidence (<80%) Link to source
PropertyValueUnitConditionsSource
Density(ρ)
0.09700
lb/in³22°C
Rows with are inherited from the base material
Verified Unverified Low confidence (<80%) Link to source

Regulatory Screening

Environmental

Safety & Biocompatibility

Quality & Standards

RoHS, REACH, and Prop 65 statuses are validated against official substance lists (ECHA SVHC Candidate List, OEHHA Prop 65, RoHS Annex II). Other regulations are estimated from composition and material classification. All screening is a starting point for due diligence — always verify with your supplier before making compliance decisions.