5086-H32 is a non-heat-treatable aluminum-magnesium alloy (approximately 3.5-4.5% Mg) strain-hardened to H32 temper, providing moderate strength with excellent seawater corrosion resistance suitable for marine structures, pressure vessels, and welded aerospace components. The H32 condition (half-hard after strain-hardening and stress relief) balances strength and ductility for applications requiring good formability while maintaining corrosion performance in salt-water and chemical environments.
Compliance & Regulations
8 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Ultimate Bearing Strength(Fbru)4 entries | 80.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · t=0.020-2.000 in · e/D=1.5 | ||
| ↳ | 82.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · t=0.020-2.000 in · e/D=1.5 | ||
| ↳ | 39.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · t=0.020-2.000 in · e/D=2 | ||
| ↳ | 42.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · t=0.020-2.000 in · e/D=2 | ||
Bearing Yield Strength(Fbry)2 entries | 48.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · t=0.020-2.000 in · e/D=1.5 | ||
| ↳ | 51.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · t=0.020-2.000 in · e/D=1.5 | ||
Compressive Modulus(Ec) | 10,400 | ksi | 22°C · Sheet/Plate | ||
Compressive Tangent Modulus vs Stress(Etn(σ))2 entries | Curve (16 pts) | ksi | 21°C · L | ||
| ↳ | Curve (15 pts) | ksi | 21°C · LT | ||
Compressive Yield Strength(Fcy) | 24.00 – 30.00 | ksi | 6 entriesClick to expand | ||
Poisson's Ratio(ν) | 0.3300 | - | 22°C | ||
Shear Modulus(G) | 3,850 | ksi | 22°C · Sheet/Plate | ||
Ultimate Shear Strength(Fsu)2 entries | 58.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · t=0.020-2.000 in | ||
| ↳ | 61.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · t=0.020-2.000 in | ||
Stress–Strain Curve(σ–ε) | Curve (18 pts) | ksi | 21°C · LT | ||
Stress–Strain Curve (buckling region, ≤ 2% strain)(σ–ε (low-strain)) | — | ksi | 5 entriesClick to expand | ||
Ultimate Tensile Strength(σUTS)4 entries | 40.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · L · t=0.020-2.000 in | ||
| ↳ | 41.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · L · t=0.020-2.000 in | ||
| ↳ | 40.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · LT · t=0.020-2.000 in | ||
| ↳ | 41.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · LT · t=0.020-2.000 in | ||
Yield Strength (0.2% offset)(σy)4 entries | 28.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · L · t=0.020-2.000 in | ||
| ↳ | 30.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · L · t=0.020-2.000 in | ||
| ↳ | 26.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · LT · t=0.020-2.000 in | ||
| ↳ | 28.00 | ksi | 22°C · Sheet/Plate · H32 · AMS-QQ-A-250/7 · LT · t=0.020-2.000 in | ||
Young's Modulus(E) | 10,200 | ksi | 22°C · Sheet/Plate | ||
2 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
CTE vs Temperature(α(T)) | Curve (17 pts) | µin/in·°F | — | ||
Thermal Conductivity vs Temperature(k(T)) | Curve (20 pts) | BTU/(hr·ft·°F) | — |
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Density(ρ) | 0.09600 | lb/in³ | 22°C |