300M is a chromium-molybdenum-vanadium alloy steel (AISI 4340-type) used in high-strength aerospace applications including landing gear, fasteners, and structural components, offering tensile strengths of 1650–1900 MPa with excellent fatigue resistance and fracture toughness when properly heat-treated.
Compliance & Regulations
35 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Ultimate Bearing Strength(Fbru)4 entries | 414 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 270 ksi level · AMS 6417 · t=≤5.00 in · e/D=1.5 | ||
| ↳ | 506 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 270 ksi level · AMS 6417 · t=≤5.00 in · e/D=2 | ||
| ↳ | 430 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 280 ksi level · AMS 6257 OR AMS 6419 · t=≤5.00 in · e/D=1.5 | ||
| ↳ | 525 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 280 ksi level · AMS 6257 OR AMS 6419 · t=≤5.00 in · e/D=2 | ||
Bearing Yield Strength(Fbry)4 entries | 344 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 270 ksi level · AMS 6417 · t=≤5.00 in · e/D=1.5 | ||
| ↳ | 379 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 270 ksi level · AMS 6417 · t=≤5.00 in · e/D=2 | ||
| ↳ | 360 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 280 ksi level · AMS 6257 OR AMS 6419 · t=≤5.00 in · e/D=1.5 | ||
| ↳ | 396 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 280 ksi level · AMS 6257 OR AMS 6419 · t=≤5.00 in · e/D=2 | ||
Compressive Modulus(Ec) | 29,000 | ksi | 22°C | ||
Compressive Yield Strength(Fcy)2 entries | 236 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 270 ksi level · AMS 6417 · t=≤5.00 in | ||
| ↳ | 247 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 280 ksi level · AMS 6257 OR AMS 6419 · t=≤5.00 in | ||
Elongation at Break(εf)2 entries | 8.000 | % | 22°C · Bar/Forging/Tubing · Quenched and tempered, 270 ksi level · AMS 6417 · L · t=≤5.00 in | ||
| ↳ | 7.000 | % | 22°C · Bar/Forging/Tubing · Quenched and tempered, 280 ksi level · AMS 6257 OR AMS 6419 · L · t=≤5.00 in | ||
Fatigue Crack Growth Rate(da/dN)3 entries | Curve (5 pts) | m/cycle | 21°C · R = 0.5 · (TUS: 280-290 ksi (1930-2000 MPa)) | ||
| ↳ | Curve (7 pts) | m/cycle | 21°C · R = 0.3 · (TUS: 280-290 ksi (1930-2000 MPa)) | ||
| ↳ | Curve (9 pts) | m/cycle | 21°C · R = 0.08 · (TUS: 280-290 ksi (1930-2000 MPa)) | ||
Poisson's Ratio(ν) | 0.3200 | - | 22°C | ||
Shear Modulus(G) | 11,000 | ksi | 22°C | ||
Ultimate Shear Strength(Fsu)2 entries | 162 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 270 ksi level · AMS 6417 · t=≤5.00 in | ||
| ↳ | 168 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 280 ksi level · AMS 6257 OR AMS 6419 · t=≤5.00 in | ||
S–N Curve (Wöhler)(S–N) | — | ksi | 28 entriesClick to expand | ||
Ultimate Tensile Strength(σUTS)4 entries | 270 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 270 ksi level · AMS 6417 · t=≤5.00 in | ||
| ↳ | 280 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 280 ksi level · AMS 6257 OR AMS 6419 · t=≤5.00 in | ||
| ↳ | Curve (12 pts) | ksi | L | ||
| ↳ | Curve (12 pts) | ksi | L | ||
Yield Strength (0.2% offset)(σy)4 entries | 220 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 270 ksi level · AMS 6417 · t=≤5.00 in | ||
| ↳ | 230 | ksi | 22°C · Bar/Forging/Tubing · Quenched and tempered, 280 ksi level · AMS 6257 OR AMS 6419 · t=≤5.00 in | ||
| ↳ | Curve (14 pts) | ksi | L | ||
| ↳ | Curve (14 pts) | ksi | L | ||
Young's Modulus(E) | 29,000 | ksi | 22°C | ||
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Density(ρ) | 0.2830 | lb/in³ | 22°C |
Reference data from cited sources. Not verified or certified by MatWorld Inc. Verify against the source before use in design. Terms: engineering data