2219 aluminum alloy (Cu-Mn primary alloying elements) is a high-strength aerospace material used in cryogenic tankage and structural applications requiring superior strength at low temperatures. The T852 temper (solution heat-treated, stress-relieved, and artificially aged) provides excellent damage tolerance and fracture toughness combined with high yield and tensile strength, making it suitable for critical pressure vessels and cryogenic service in hand-forged form per AMS 4144.
Compliance & Regulations
21 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Ultimate Bearing Strength(Fbru)4 entries | 80.00 | ksi | 22°C · Hand Forging · T852 · AMS 4144 · t=6.001-8.000 in · e/D=1.5 | ||
| ↳ | 104 | ksi | 22°C · Hand Forging · T852 · AMS 4144 · t=2.000-4.000 in · e/D=2 | ||
| ↳ | 100 | ksi | 22°C · Hand Forging · T852 · AMS 4144 · t=4.001-6.000 in · e/D=2 | ||
| ↳ | 102 | ksi | 22°C · Hand Forging · T852 · AMS 4144 · t=6.001-8.000 in · e/D=2 | ||
Bearing Yield Strength(Fbry) | 64.00 – 89.00 | ksi | 6 entriesClick to expand | ||
Compressive Modulus(Ec) | 10,800 | ksi | 22°C · Extruded shapes | ||
Compressive Tangent Modulus vs Stress(Etn(σ)) | — | ksi | 6 entriesClick to expand | ||
Compressive Yield Strength(Fcy) | 39.00 – 47.00 | ksi | 9 entriesClick to expand | ||
Elongation at Break(εf) | 2.000 – 6.000 | - | 23 entriesClick to expand | ||
Poisson's Ratio(ν) | 0.3300 | - | 22°C | ||
Shear Modulus(G) | 4,000 | ksi | 22°C · Extruded shapes | ||
Ultimate Shear Strength(Fsu) | 32.00 – 37.00 | ksi | 9 entriesClick to expand | ||
Stress–Strain Curve(σ–ε)3 entries | Curve (14 pts) | ksi | 21°C · L | ||
| ↳ | Curve (13 pts) | ksi | 21°C · LT | ||
| ↳ | Curve (14 pts) | ksi | 21°C · ST | ||
Stress–Strain Curve (buckling region, ≤ 2% strain)(σ–ε (low-strain)) | — | ksi | 12 entriesClick to expand | ||
Ultimate Tensile Strength(σUTS) | 50.00 – 62.00 | ksi | 23 entriesClick to expand | ||
Yield Strength (0.2% offset)(σy) | 37.00 – 50.00 | ksi | 23 entriesClick to expand | ||
Young's Modulus(E) | 10,500 | ksi | 22°C · Extruded shapes | ||
3 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
CTE vs Temperature(α(T)) | Curve (13 pts) | µin/in·°F | — | ||
Specific Heat vs Temperature(Cp(T)) | Curve (15 pts) | BTU/(lb·°F) | — | ||
Thermal Conductivity vs Temperature(k(T)) | Curve (11 pts) | BTU/(hr·ft·°F) | — |
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Density(ρ) | 0.1030 | lb/in³ | 22°C |