2014 aluminum is a copper-alloyed high-strength aluminum used primarily in aircraft structural forgings and landing gear components, offering tensile strengths in the 60–70 ksi range with good fatigue resistance. The T652 temper (solution heat-treated, stress-relieved, and artificially aged) provides dimensional stability and controlled strength suitable for precision forged parts requiring consistent mechanical properties and minimal distortion.
Compliance & Regulations
13 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Ultimate Bearing Strength(Fbru) | 83.00 – 127 | ksi | 24 entriesClick to expand | ||
Bearing Yield Strength(Fbry) | 71.00 – 94.00 | ksi | 24 entriesClick to expand | ||
Compressive Modulus(Ec) | Curve (13 pts) | ksi | L | ||
Compressive Tangent Modulus vs Stress(Etn(σ))3 entries | Curve (7 pts) | ksi | 21°C · compressive · T652 · L | ||
| ↳ | Curve (7 pts) | ksi | 21°C · compressive · T652 · LT | ||
| ↳ | Curve (8 pts) | ksi | 21°C · compressive · T652 · ST | ||
Compressive Yield Strength(Fcy) | 53.00 – 62.00 | ksi | 28 entriesClick to expand | ||
Elongation at Break(εf) | 1.000 – 8.000 | % | 29 entriesClick to expand | ||
Fracture Toughness(KIC)2 entries | 31.00 range 24.00–48.00 | ksi·√in | 22°C · Hand Forging · T652 · L-T · t=≥0.5 in | ||
| ↳ | 21.00 range 18.00–30.00 | ksi·√in | 22°C · Hand Forging · T652 · T-L · t=≥0.8 in | ||
Poisson's Ratio(ν) | 0.3300 | - | 22°C | ||
Shear Modulus(G) | 4,000 | ksi | 22°C · Hand forging | ||
Ultimate Shear Strength(Fsu) | 36.00 – 41.00 | ksi | 12 entriesClick to expand | ||
Stress–Strain Curve(σ–ε)2 entries | Curve (9 pts) | ksi | 21°C · T652 · LT | ||
| ↳ | Curve (10 pts) | ksi | 21°C · T652 · L | ||
Stress–Strain Curve (buckling region, ≤ 2% strain)(σ–ε (low-strain)) | — | ksi | 6 entriesClick to expand | ||
Ultimate Tensile Strength(σUTS) | 57.00 – 67.00 | ksi | 31 entriesClick to expand | ||
Yield Strength (0.2% offset)(σy) | 48.00 – 59.00 | ksi | 31 entriesClick to expand | ||
Young's Modulus(E) | Curve (13 pts) | ksi | L | ||
3 interactive curves for this material
Stress-strain, S-N fatigue and environmental knockdown curves are free with an account.
Create free account| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
CTE vs Temperature(α(T)) | Curve (9 pts) | µin/in·°F | T6 | ||
Specific Heat vs Temperature(Cp(T)) | Curve (4 pts) | BTU/(lb·°F) | T6 | ||
Thermal Conductivity vs Temperature(k(T)) | Curve (8 pts) | BTU/(hr·ft·°F) | T6 |
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Density(ρ) | 0.1010 | lb/in³ | 22°C |
Reference data from cited sources. Not verified or certified by MatWorld Inc. Verify against the source before use in design. Terms: engineering data