17-4PH stainless steel printed by metal binder jetting is a precipitation-hardening martensitic steel formed by depositing binder into a powder bed, then debinding and sintering the part. The green part is fragile and porous and shrinks substantially in sintering, so geometry is scaled to compensate and long spans may need setters. Some residual porosity usually remains, the surface is that of sintered powder, and critical features are often machined. Residual stress and anisotropy are low compared with fusion processes, and final strength depends on sintering and the later aging treatment. It is used for production runs of complex brackets, housings, fittings and tooling.
Compliance & Regulations
Each row is one condition this material was measured in. Its values and curves are in the tables and charts below, labelled with the condition; the ranges here span that row's own cited values and are never averaged across rows.
| Condition | Yield (MPa) | UTS (MPa) | Elongation (%) | E (GPa) | Density (kg/m³) | Values | Curves |
|---|---|---|---|---|---|---|---|
| Desktop Metal 17-4PH Stainless Steel (Shop System), heat-treated | 931–1058 | 1170–1240 | 5.9–16.9 | 165–205 | 7500–7660 | 13 | 0 |
| Desktop Metal 17-4PH Stainless Steel (Shop System), sintered | 620–820 | 845–1005 | 3.9–12.7 | 148–208 | 7500–7700 |
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Charpy Impact Energy(KV)4 entries | 158 range 151–165 | J | Desktop Metal 17-4PH Stainless Steel (Shop System), heat-treated · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · heat-treated · MPIF 59 | ||
| ↳ | 152 range 147–157 | J | Desktop Metal 17-4PH Stainless Steel (Shop System), heat-treated · MECHANICAL PROPERTIES SINTERED IN THIRD-PARTY COMMERCIAL FURNACE · heat-treated · MPIF59 · XY | ||
| ↳ | 107 range 93.00–121 | J | Desktop Metal 17-4PH Stainless Steel (Shop System), sintered · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · sintered · MPIF 59 | ||
| ↳ | 150 range 142–158 | J | Desktop Metal 17-4PH Stainless Steel (Shop System), sintered · MECHANICAL PROPERTIES SINTERED IN THIRD-PARTY COMMERCIAL FURNACE · sintered · MPIF59 · XY | ||
Elongation at Break(εf)4 entries | 8.900 range 5.900–11.90 | % | Desktop Metal 17-4PH Stainless Steel (Shop System), heat-treated · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · heat-treated · ASTM E8M · XY | ||
| ↳ | 11.90 range 6.900–16.90 | % | Desktop Metal 17-4PH Stainless Steel (Shop System), heat-treated · MECHANICAL PROPERTIES SINTERED IN THIRD-PARTY COMMERCIAL FURNACE · heat-treated · ASTM E8M | ||
| ↳ | 10.40 range 8.100–12.70 | % | Desktop Metal 17-4PH Stainless Steel (Shop System), sintered · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · sintered · ASTM E8M · XY | ||
| ↳ | 5.900 range 3.900–7.900 | % | Desktop Metal 17-4PH Stainless Steel (Shop System), sintered · MECHANICAL PROPERTIES SINTERED IN THIRD-PARTY COMMERCIAL FURNACE · sintered · ASTM E8M | ||
Hardness (Rockwell C)(HRC)4 entries | 38.70 range 37.30–40.10 | HRC | Desktop Metal 17-4PH Stainless Steel (Shop System), heat-treated · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · heat-treated · ASTM E18 | ||
| ↳ | 40.50 range 38.50–42.50 | HRC | Desktop Metal 17-4PH Stainless Steel (Shop System), heat-treated · MECHANICAL PROPERTIES SINTERED IN THIRD-PARTY COMMERCIAL FURNACE · heat-treated · ASTM E18 | ||
| ↳ | 26.00 range 24.70–27.30 | HRC | Desktop Metal 17-4PH Stainless Steel (Shop System), sintered · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · sintered · ASTM E18 | ||
| ↳ | 26.40 range 25.40–27.40 | HRC | Desktop Metal 17-4PH Stainless Steel (Shop System), sintered · MECHANICAL PROPERTIES SINTERED IN THIRD-PARTY COMMERCIAL FURNACE · sintered · ASTM E18 | ||
Ultimate Tensile Strength(σUTS)4 entries | 174.8 range 172.2–177.4 | ksi | Desktop Metal 17-4PH Stainless Steel (Shop System), heat-treated · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · heat-treated · ASTM E8M · XY | ||
| ↳ | 174.8 range 169.7–179.8 | ksi | Desktop Metal 17-4PH Stainless Steel (Shop System), heat-treated · MECHANICAL PROPERTIES SINTERED IN THIRD-PARTY COMMERCIAL FURNACE · heat-treated · ASTM E8M | ||
| ↳ | 134.2 range 122.6–145.8 | ksi | Desktop Metal 17-4PH Stainless Steel (Shop System), sintered · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · sintered · ASTM E8M · XY | ||
| ↳ | 132.3 range 127.2–137.4 | ksi | Desktop Metal 17-4PH Stainless Steel (Shop System), sintered · MECHANICAL PROPERTIES SINTERED IN THIRD-PARTY COMMERCIAL FURNACE · sintered · ASTM E8M | ||
Yield Strength (0.2% offset)(σy)4 entries | 147.9 range 142.4–153.4 | ksi | Desktop Metal 17-4PH Stainless Steel (Shop System), heat-treated · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · heat-treated · ASTM E8M · XY | ||
| ↳ | 142.3 range 135–149.5 | ksi | Desktop Metal 17-4PH Stainless Steel (Shop System), heat-treated · MECHANICAL PROPERTIES SINTERED IN THIRD-PARTY COMMERCIAL FURNACE · heat-treated · ASTM E8M | ||
| ↳ | 105.9 range 92.82–118.9 | ksi | Desktop Metal 17-4PH Stainless Steel (Shop System), sintered · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · sintered · ASTM E8M · XY | ||
| ↳ | 95.72 range 89.92–101.5 | ksi | Desktop Metal 17-4PH Stainless Steel (Shop System), sintered · MECHANICAL PROPERTIES SINTERED IN THIRD-PARTY COMMERCIAL FURNACE · sintered · ASTM E8M | ||
Young's Modulus(E)4 entries | 28,572.4 | ksi | Desktop Metal 17-4PH Stainless Steel (Shop System), heat-treated · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · heat-treated · ASTM E111 · XY | ||
| ↳ | 26,832 range 23,931.2–29,732.7 | ksi | Desktop Metal 17-4PH Stainless Steel (Shop System), heat-treated · MECHANICAL PROPERTIES SINTERED IN THIRD-PARTY COMMERCIAL FURNACE · heat-treated · ASTM E8M | ||
| ↳ | 27,702.2 | ksi | Desktop Metal 17-4PH Stainless Steel (Shop System), sintered · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · sintered · ASTM E111 · XY | ||
| ↳ | 25,816.7 range 21,465.6–30,167.9 | ksi | Desktop Metal 17-4PH Stainless Steel (Shop System), sintered · MECHANICAL PROPERTIES SINTERED IN THIRD-PARTY COMMERCIAL FURNACE · sintered · ASTM E8M |
| Property | Value | Unit | Conditions | Source | |
|---|---|---|---|---|---|
Density(ρ)4 entries | 0.2738 range 0.2710–0.2767 | lb/in³ | Desktop Metal 17-4PH Stainless Steel (Shop System), heat-treated · MECHANICAL PROPERTIES SINTERED IN THIRD-PARTY COMMERCIAL FURNACE · heat-treated · ASTM B311 | ||
| ↳ | 0.2775 range 0.2767–0.2782 | lb/in³ | Desktop Metal 17-4PH Stainless Steel (Shop System), sintered · MECHANICAL PROPERTIES IN DESKTOP METAL PURESINTER FURNACE · sintered · ASTM B311 | ||
| ↳ | 0.2738 range 0.2710–0.2767 | lb/in³ | Desktop Metal 17-4PH Stainless Steel (Shop System), sintered · MECHANICAL PROPERTIES SINTERED IN THIRD-PARTY COMMERCIAL FURNACE · sintered · ASTM B311 | ||
| ↳ | 0.2820 | lb/in³ | 22°C |
Reference data from cited sources. Not verified or certified by MatWorld Inc. Verify against the source before use in design. Terms: engineering data
| 14 |
| 0 |
Machines the manufacturer states for this material.